Ignition Activation Energy of Materials based on Polyamide 6

Peter Rantuch, Igor Wachter, Ivan Hrušovský, Karol Balog
Transactions of the VSB - Technical University of Ostrava, Safety Engineering Series
2016, Volume 11, Issue 1, Pages 27-31
Doi: 10.1515/tvsbses-2016-0004
This contribution is aimed to compare the values of the ignition activation energies of two types of polyamide – Slovamid 6 FRB and Slovamid GF 50 LTS. Samples were isothermally stressed at five different temperatures between 500°C a 550°C, while the time to initiation of the flame combustion was monitored. Subsequently from the measured times were compiled Arrhenius plots under which activation energy of ignition of both polymers were calculated. The values of activation energies were 106 kJ/mol and 158.0 kJ/mol for Slovamid 6 FRB 4 and Slovamid 6 GF 50 LTS.